Our pigment can be applied to make photoluminescent ceramic
glaze directly. Following content is some information about the method of making
photoluminesent ceramic glaze for your reference.
1.Make the based normal
transparent ceramic glaze.The glaze should be ground thin,can through the
250mesh sieve.
2.Mixing well the photoluminescent pigment and the based
ceramic glaze by the proportion of 4:6 to make the luminous ceramic glaze.
3.During the production,don't let the photoluminescent pigment touch with
the metal material,otherwise the luminous effect will be affected
Use of
Luminous Glaze of Pottery
1. Luminous glaze on the surface of internal brick
wall
(1) Mix TGB-45M luminous glaze of pottery and water in the ratio of 1:
0.6—0.7 in ball grinding machine for about 20 minutes to prepare glair.
(2)
Use the way of spreading, pouring and dropping glaze on the pottery blanks to
form 200---400μm glaze layer.
(3) Let them dry.
(4) Quickly bake them for
35—50minutes with a temperature of 1000--1080℃ to get the glaze surface bricks
that used on internal wall. 2. Luminous Ground Brick
(with designs)
(1) Mix evenly TGB—45H luminous glaze of pottery and proper
meshwork oil to get meshwork printing slurry.
(2) Print luminous glair using
meshwork on the surface bricks with white unbaked glaze layer to form luminous
designs.
(3) Pour transparent glair on the surface of designs.
(4) Bake
them for 35—45 minutes with a temperature of 1100--1180℃ to get ground bricks
with luminous designs. 3. Internal Wall
Bricks with Luminous Design (Baked for three times)
(1) Mix TGB—45L luminous
glair of pottery with proper printing oil of meshwork to prepare slurry for
meshwork printing.
(2) Print luminous designs on the surface of baked bricks
with white glaze.
(3) Pile transparent dry glaze powder on the luminous
designs with meshwork.
(4) Bake them for 40—45 minutes with a temperature
900---1000℃ to get bulgy designs on the bricks for decoration of internal
wall.
Notice:
1. Avoid attrition between luminous glaze and metals, or will
influence luminous effects.
2. if there is settle in glair, add 2% pengrun
earth to increase suspension of glair.
3. The preferential product applied is
the transparent glaze produced by our corporation.